Investigation and effect of PVC and PVTMS on sintering, physical
and mechanical features of chipboard wood
Roghaiyeh Mazloumihaghghi
Department of agricultural and mechanical engineering, Science and Research Branch, Islamic
Azad University, Tehran, Iran
DOI : https://doi.org/10.51583/IJLTEMAS.2024.130506
Received: 20 April 2024; Accepted: 30 April 2024; Published: 08 June 2024
Abstract: Due to their unique combination of properties, wood-plastic composites (WPC) have proven to be a promising
alternative to conventional wood and plastic materials in various applications. This article provides a new insight into WPCs
consisting of chipboard wood as matrix and polyvinyl chloride (PVC) and poly vinyl trimtehoxy silane (PVTMS) as
reinforcement. Overall, this paper highlights the significant advances and opportunities in the field of wood-polymer composites
and their potential as sustainable, high-performance materials with a wide range of applications. Continuous research and
development efforts are essential to further improve the properties and expand the use of WPC in various industries. In the
manufacturing process, wood and thermoplastic polymers are blended together, often using additives and binders to improve
compatibility and performance. The resulting composites have desirable properties, such as a high strength-to-weight ratio and
the ability to be molded into complex shapes. The differential scanning calorimetry (DSC), flourier transform infrared (FTIR), X-
Ray diffraction (XRD), X-ray photoelectron spectroscopy and scanning Electron Microscopy (SEM) characteristics and
mechanical properties were discussed in detail. As a result, the composite material sintered at 80 showed better mechanical
behavior, with the compressive strength calculated to be 28.73 MPa.
Keywords: Chipboard wood; composites; PVC; PVTMS; Mechanical behavior
I. Introduction
Chipboard wood, also known as chipboard, is a type of wood-based material made from wood shavings, sawdust or sawdust
together with a synthetic resin or binder[1]. These materials are compressed and bonded together under high pressure and heat to
form panels[2]. Chipboard is often used in construction, furniture manufacturing and interior design due to its affordability,
versatility and ease of processing[3]. The manufacturing process begins with the wood raw materials being mixed with resin and
additives in a mixer. The mixture is then spread out in a continuous mat or layered in a mold box[3]. Hydraulic presses apply
pressure and heat, usually between 140 and 220 , to compress the material and cure the resin, creating a dense and uniform
board[4]. The density and properties of particleboard depend on factors such as the size and type of wood particles used, the resin
content and the manufacturing process. Low density chipboard is often used for packaging, while higher density chipboard is
suitable for furniture, cabinets, flooring and wall panels. Despite its affordability and versatility, chipboard has some limitations
compared to solid wood or other wood-based materials[5]. They tend to swell and warp when exposed to moisture, and their
strength and durability can be less than that of plywood or oriented strand board (OSB)[6]. However, with the right finishing and
protective coating, chipboard can be used effectively in a variety of applications and is a cost-effective and sustainable alternative
to solid wood. Wood plastic nano-composites (WPC) have attracted a great deal of attention in recent years as a sustainable
alternative to conventional materials in various industries[7]. This innovative nano-composite material combines the natural
esthetics and structural properties of wood with the durability and versatility of plastics[8]. The development of WPCs has been
driven by the need for environmentally friendly materials that offer better performance, durability and reduced environmental
impact compared to conventional wood or plastic products[9]. The concept of combining wood fibers or flour with thermoplastic
polymers emerged in the 1980s, and since then WPCs have evolved into a diverse class of materials with a wide range of
applications[10]. The manufacturing process typically involves blending wood particles or fibers with polymers such as
polyethylene, polypropylene or polyvinyl chloride, as well as additives and bonding agents to improve compatibility and
performance[11]. This mixture is then formed into various shapes using processes such as extrusion, injection molding or
compression molding. One of the main advantages of WPCs is the balance of their properties, that are superior to those of wood
and plastic alone[12]. These include resistance to moisture, rot and insects, dimensional stability, low maintenance and the ability
to form complex shapes[13]. WPCs are therefore used in various industries, e.g. construction, automotive, furniture, landscaping
and consumer goods. In addition, WPCs contribute to sustainability efforts as they are made from recycled materials, reduce the
need for virgin plastics and wood and are recyclable at the end of their life cycle[14]. However, challenges such as long-term
durability, material variability and recyclability still require further research and development[15]. In summary, wood-plastic
nano-composites are a promising solution for sustainable material innovation as they offer a compelling combination of natural
esthetics, performance and environmental benefits. With further advances in manufacturing processes, material formulations and
end-of-life options, WPCs have the potential to revolutionize various industries while reducing their environmental
footprint[16].Polyvinyl chloride (PVC) is a synthetic polymer used in numerous applications due to its versatility, durability and
cost-effectiveness[17]. It is one of the most widely produced and used plastics in the world. PVC is produced by the
polymerization of vinyl chloride monomers. PVC comes in two main forms: Rigid and flexible PVC. Rigid PVC, often referred
to as PVC-U (soft PVC), is often used in the construction industry for pipes, window frames and cladding due to its excellent
INTERNATIONAL JOURNAL OF LATEST TECHNOLOGY IN ENGINEERING,
MANAGEMENT & APPLIED SCIENCE (IJLTEMAS)
ISSN 2278-2540 | DOI: 10.51583/IJLTEMAS | Volume XIII, Issue V, May 2024
www.ijltemas.in Page 39
strength, chemical resistance and flame tendency[18]. Flexible PVC, also known as soft PVC, contains additional plasticizers to
give it flexibility and is used for applications such as vinyl flooring, cables, hoses and medical tubing[19]. One of the main
advantages of PVC is its durability. It is resistant to moisture, weather, chemicals and abrasion, making it suitable for use
outdoors and in harsh environments[20]. PVC is also relatively lightweight, easy to work with and has good electrical insulation
properties. Poly Vinyl trimethoxy silane (PVTMS) is a chemical compound that belongs to the organo silane family[21]. These
are organ functional silanes that are used in various industrial applications, particularly in materials science and surface
modification processes. PVTMS consists of a vinyl group (C
2
H
3
), which provides reactivity, and three methoxy groups (C
2
H
3
)
bonded to a silicon atom (Si), as well as a trimethylsilyl group. PVTMS is generally used as an adhesion promoter in the
modification of surfaces, especially surfaces made of inorganic materials such as glass, ceramics or metals[22]. It is used to
improve the compatibility between organic polymers and inorganic substrates by forming covalent bonds with hydroxyl groups
on the surface. This leads to improved adhesion, wetting and bonding properties[23]. In addition to surface modification, PVTMS
is also used as a crosslinking agent in the synthesis of organic-inorganic hybrid materials, where it facilitates the formation of
covalent bonds between organic polymers and inorganic nanoparticles or fillers[24],[25]. This can lead to the development of
nano-composite materials with improved mechanical, thermal or barrier properties. In addition, PVTMS is used in the production
of functional coatings, sealants and adhesives, where it provides adhesion and durability to the treated surfaces. It is also used in
the production of silicone-based materials, where it serves as a precursor for the synthesis of siloxane polymers. Overall, PVTMS
plays a crucial role in surface modification, crosslinking and the development of advanced materials, helping to improve
performance and functionality in various industrial applications. In this study, 90 wt.% chipboard wood and 5 wt.% of PVC and
5wt% of PVTMS were utilized to prepare two types of nano-composites sintered at 50 °C and 80 °C, respectively.
II. Materials and methods
Chipboard wood is made from reconstituted wood-often shavings, shavings or sawdust - which is compressed and held
together with natural or synthetic resin and then formed into panels. It became popular thanks to its low price, as it's much
cheaper than normal, pure wood such as pine or oak. PVC and VTMS were manufactured by Merck. Differential scanning
calorimetry (DSC) is an analytical method for measuring the heat flow associated with thermal transitions in materials as a
function of temperature. The STA-BAHR DSC was used. Fourier transform infrared spectroscopy (FTIR) of the compounds
were performed in the potassium bromide (KBr) powders, and the instrument was the Perkin-Elmer Spectrum BX FT-IR
spectrometer. X-ray diffraction were performed at 40 kV and 40 mA and recorded from 20 to 50 degrees for at a scan rate
of 2.5 degrees/minute and an increment of 0.02 degrees. The resulting patterns were analyzed with the High Score X’Pert
software using the procedure implemented in the ASC suffix files for basic parameters. To study the morphology of the
samples, the XPS UHV analysis system was selected and the Phillips/FEI Quanta 200 scanning electron microscope (SEM)
analysis was used. SANTAM STM-50 and H-25KT were used to study the mechanical properties and the samples were
prepared according to the ASTM-E9 standard.
a. Synthesis and merge of PVC and PVTMS
PVC and VTMS were mixed and tertiary butyl peroxide was considered as initiator under reflux and stirred for 6 hours at 60 °C
in flowing nitrogen. In addition, the chemical structures of PVC and PVTMS are shown in Scheme 1[23].
Schematic 1. Chemical structures of PVC and PVTMS
III. Result and discussion
a. Thermal investigation
The DSC analysis of the nano-composites was performed and as a result the thermal curve is shown in Figure 1. The
endothermic temperature ranges at 196 of chipboard wood can be associated with this, indicating a high amount of water
molecules and the removal of the external water or bulk water inside the structure[26]. Therefore, the resin may soften or melt
when the chipboard wood is exposed to heat before the wood particles undergo significant thermal decomposition. In addition,
INTERNATIONAL JOURNAL OF LATEST TECHNOLOGY IN ENGINEERING,
MANAGEMENT & APPLIED SCIENCE (IJLTEMAS)
ISSN 2278-2540 | DOI: 10.51583/IJLTEMAS | Volume XIII, Issue V, May 2024
www.ijltemas.in Page 40
the resin used in chipboard typically has a higher melting or softening point than the wood particles. Therefore, this endotherm
may dominate when the chipboard is exposed to heat and the resin softens or melts before the wood particles undergo significant
thermal decomposition. However, it should be noted that chipboard itself does not melt like a pure substance, but can soften,
deform or decompose under high temperatures. It is noteworthy that three thermal peaks occurred at 135, 190 and 297 by
adding PVC and PVTMS when only the heat flow area of the sintered nano-composite was increased to 80 [27]. Since the
melting point of PVC is usually between 75 and 100 °C, the removal of water and the melting of PVC occurred simultaneously at
135 [28],[29]. Therefore, the sintering temperature was not chosen to be higher than 80 . The endothermic region at 297
was attributed to the breakage of the Si-Si bond in the PVTMS structure.
Figure 1. DSC curve of chipboard wood and sintered nano-composites at 50 and 80 ℃
b. Study of FTIR and X-ray diffraction
According to the FTIR spectra of chipboard wood and sintered nano-composites at 50 and 80 (Figure 2-a), the resulting
spectrum represents the unique fingerprint of the sample's chemical composition. The FTIR spectrum of chipboard wood
(black dash) can provide valuable information about the chemical composition, including the type of wood used, the presence
of additives or binders (e.g. resins) and any chemical changes due to manufacturing processes. This information can be useful
for quality control, process optimization and understanding the properties of chipboard wood in various applications[30].
Hydroxyl (OH), carbonyl (C=O), methylene (CH
2
) and aromatic (C=C) groups. In addition, the C-H stretching vibrations of
the vinyl group (CH=CH
2
) typically occur at 3000-3300 1/cm in the FTIR of the nano-composites[31]. In addition, the small
and inconspicuous CH stretching vibrations of the (CH
2
) groups typically occur at 1800-2400 1/cm. The C=O stretching
vibrations of the carbonyl groups (C=O) can be observed at about 1500 1/cm. For XRD analysis, the particle boards were
usually prepared by cutting or milling into small pieces to ensure uniformity and flatness. Moreover, XRD analysis of
chipboard wood can provide valuable information about its composition, including the types and relative proportions of
minerals or crystalline phases present, as well as any structural changes due to manufacturing processes or environmental
factors. This information is useful for understanding the properties and performance of chipboard wood. The main peaks at
values of approximately (14° and 16°), (21° and 23°) and 35° are surmounted by planes (101), (002) and (311) in tandem[32].
In addition, there is no crystalline phase when the narrow and sharp peaks were not observed and the amorphous phase was
above the crystalline phase.
Figure 2. a) FTIR and b) X-ray diffraction of chipboard wood and sintered nano-composites at 50 and 80 ℃
INTERNATIONAL JOURNAL OF LATEST TECHNOLOGY IN ENGINEERING,
MANAGEMENT & APPLIED SCIENCE (IJLTEMAS)
ISSN 2278-2540 | DOI: 10.51583/IJLTEMAS | Volume XIII, Issue V, May 2024
www.ijltemas.in Page 41
c. XPS evaluation
The XPS spectrum of chipboard wood usually contains peaks corresponding to the photoelectron emissions of elements such
as carbon (C), oxygen (O), nitrogen (N) and possibly other elements present in the wood or in the surface treatment. By
analyzing the positions and intensities of these peaks, researchers can identify the elemental composition of the chipboard
wood surface and gain insight into the chemical environment[33]. Overall, XPS analysis is a powerful tool for characterizing
the surface chemistry of chipboard wood and gaining insight into its composition and properties at the atomic level. The XPS
spectrum of chipboard wood typically contains peaks corresponding to the core-level photoelectron transitions of elements
such as carbon (C 1s), oxygen (O 1s), nitrogen (N 1s) and possibly other elements, depending on the specific composition of
the wood and any surface treatments or impurities present[34]. By analyzing the positions, shapes and intensities of these
peaks, researchers can identify the elements present and gain insight into their chemical environments and bonding states. XPS
analysis of chipboard wood can provide valuable information about the surface chemistry of the material, including the
presence of organic constituents (such as cellulose, lignin and resins) as well as surface treatments, impurities or degradation
products. Furthermore, in nano-composites, the binding energy of the C 1s peak associated with CCl bonds in PVC is
typically lower than that of the C 1s peak associated with CC bonds, reflecting the different chemical environments of these
carbon atoms[35]. In nano-composites, carbon-carbon (CC) bonds typically have binding energy values around 283 eV.
Carbon-chlorine (CCl) bonds have lower binding energy values compared to CC bonds due to the electron-withdrawing
nature of chlorine atoms. The binding energy values for CCl bonds in PVC can vary depending on factors such as the degree
of chlorination and the local chemical environment. Carbon-oxygen (CO) bonds[36]. Also, the binding energy values for Cl
2p in PVC are also around 284.3 eV and reflect the chemical environment of the chlorine atoms bonded to carbon atoms in the
polymer chain[37],[38].
Figure 3. XPS curve of chipboard wood and sintered nano-composites at 50 and 80
d. Investigation of morphology
SEM analysis (Figure 4) of chipboard wood and nano-composites can provide valuable information about the distribution,
size, shape and organization of wood particles as well as pores, voids or defects in the material. Furthermore, SEM analysis
can help to identify the presence of additional components such as resin binders or additives and investigate their distribution
within the chipboard matrix. SEM images can reveal surface features such as cracks, fractures, delamination and surface
roughness. These features can be caused by manufacturing processes, environmental influences or mechanical stress[39]. The
surface characteristics can provide information about the durability, wear resistance and aging behavior of chipboard wood and
nano-composite materials. Porosity was observed in sintered nano-composites at 50 more than 80 , and the sintering
temperature had a very strong effect on the morphology, as the content of porosity was reduced with increasing sintering
treatment. Shiny cracks were not observed in the composites, but were observed in the particleboards (Figure 4-a). During the
manufacturing process of composites, the wood particles are bound together with resins, creating voids between the particles
that can contribute to the porous structure of the material[39]. Overall, the presence of porosity in the SEM images of these
nano-composites is a common feature resulting from the natural structure of the material, processing conditions, composition
and environmental factors[40]. Understanding the factors that contribute to porosity is essential for assessing the
microstructure and properties of chipboard and optimizing its performance in various applications.
INTERNATIONAL JOURNAL OF LATEST TECHNOLOGY IN ENGINEERING,
MANAGEMENT & APPLIED SCIENCE (IJLTEMAS)
ISSN 2278-2540 | DOI: 10.51583/IJLTEMAS | Volume XIII, Issue V, May 2024
www.ijltemas.in Page 42
Figure 4. SEM images of [a) chipboard wood], [b), c), d), e), f) sintered nano-composites at 50 ℃] and [g), h), i), j), k) sintered
nano-composites at 80 ℃] at different magnifications
e. Stress-strain curve of samples
Here is a general overview, elastic range, in the initial phase of loading, chipboard wood behaves elastically, i.e. it deforms
reversibly under the applied stress. This elastic deformation is generally linear and can be described by Hooke's law[41],[42].
The material returns to its original shape as soon as the load is removed. In the yield range, chipboard wood can deform
plastically with increasing stress, especially in areas where the resin bond between the particles begins to fail or when local
buckling occurs. This leads to a deviation from the linearity of the stress-strain curve. In the failure region, nano-composites
reach their ultimate strength, beyond which they deform significantly or fail. This failure can manifest itself as crushing,
cracking, splitting or delamination of the material, depending on the specific conditions and load configuration. The stress-
strain-compression curve of the samples is shown in Figure 5. The maximum value of compressive strength was measured at
28.73 MPa at a strain of ~ 2. According to Hooke's law, the elasticity coefficient was calculated to be ~ 4.96 MPa when
selecting the difference values of two points in the elastic region, and this value is higher than chipboard wood when the
polymers were added as reinforcement. The material returns to its original shape as soon as the load is removed, and the strain
is directly proportional to the stress according to Hooke's law. The behavior of chipboard wood under increasing load depends
on several factors, including composition, density, moisture content, resin type and manufacturing process. It's important to
understand the mechanical properties of the material and its response to stress to ensure its performance and durability in
practical applications. Experimental tests, such as tensile or compression tests, can provide valuable data on the behavior of the
material under different loading conditions.
INTERNATIONAL JOURNAL OF LATEST TECHNOLOGY IN ENGINEERING,
MANAGEMENT & APPLIED SCIENCE (IJLTEMAS)
ISSN 2278-2540 | DOI: 10.51583/IJLTEMAS | Volume XIII, Issue V, May 2024
www.ijltemas.in Page 43
Figure 5. Stress-strain curve of chipboard wood and sintered nano-composites at 50 and 80 ℃
IV. Conclusions
The characterization of chipboard wood and nano-composites was discussed in detail. The incorporation of PVC and PVTMS is a
promising approach to improve the mechanical properties of chipboard and offers opportunities for the development of durable,
sustainable and high performance products in various industries. As the melting point of PVC is normally between 75 and 100 °C,
the sintering temperature was chosen to be no higher than 80 ℃. The FTIR studies showed that the bonds were in good
agreement with the precursors. The XRD of the samples showed that there is no crystalline phase in the particle boards and also
in the nano-composites. The impressive value of binding energy for Cl 2p in PVC was observed at 284.3 eV. SEM analysis
revealed that the porosity in the sintered composites at a temperature of 50 to 80 was very high due to the chemical structure
and bonding at this temperature. It has been shown that the addition of PVC and PVTMS significantly improves the mechanical
properties of wood-based materials. The composites sintered at 80 exhibited better strength than the nano-composites sintered
at 50 and the chipboard, where the maximum value of compressive strength was calculated to be 28.73 MPa. In addition to
strength, PVC and PVTMS also contribute to a significant improvement in the stiffness of wood. The nano-composites become
stiffer and can withstand higher loads without excessive deformation. This improvement in stiffness is critical for applications
that require structural integrity and dimensional stability. In summary, the effect of PVC and PVTMS on chipboard is truly
impressive, resulting in a remarkable change in mechanical properties, durability and sustainability. By utilizing the unique
properties of polymers, wood-polymer nano-composites offer versatile solutions with improved performance and functionality,
paving the way for a wide range of applications in various industries.
References
1. T. Nishimura, Chipboard, oriented strand board (OSB) and structural composite lumber, Wood Compos. (2015) 103
121. https://doi.org/10.1016/B978-1-78242-454-3.00006-8.
2. J. Shi, H. Yu, W. Qin, W. Yang, X. Zhuang, F. Rao, M. Yin, Z. Ban, Fabrication of a new bamboo composite with large-
size high-quality flattened surface, Ind. Crops Prod. 209 (2024) 117953. https://doi.org/ 10.1016/J.INDCROP. 2023.
117953.
3. P. Marchetti, A. Marcon, G. Pesce, G. Paolo, L. Guarda, V. Pironi, M.E. Fracasso, P. Ricci, R. de Marco, Children living
near chipboard and wood industries are at an increased risk of hospitalization for respiratory diseases: A prospective
study, Int. J. Hyg. Environ. Health. 217 (2014) 95101. https://doi.org/10.1016/J.IJHEH.2013.03.015.
4. G. Toscano, V. Maceratesi, E. Leoni, P. Stipa, E. Laudadio, S. Sabbatini, FTIR spectroscopy for determination of the
raw materials used in wood pellet production, Fuel. 313 (2022) 123017. https://doi.org/10.1016/J.FUEL.2021.123017.
5. H. Zhang, Z. Ling, S. Zhou, X. Fang, W. Zhang, Preparation and characteristic of wood-based inorganic composite
phase change material with effective anisotropic thermal conductivity for thermal energy storage, Sol. Energy Mater.
Sol. Cells. 251 (2023) 112172. https://doi.org/10.1016/J.SOLMAT.2022.112172.
6. S. Zheng, M. Chen, J. Wu, J. Xu, Effect of heat treatment on properties and interfacial compatibility of poplar veneer/
polyethylene film composite plywood, Polym. Test. 122 (2023) 108006. https://doi.org/10.1016/J.
POLYMERTESTING. 2023.108006.
7. J. Hong, Z. Wang, L. Li, C. Guo, Value-added utilization of corncob hydrolysis residues: Preparation of reinforced
wood-plastic composite with highly water resistance and decay resistance, Ind. Crops Prod. 195 (2023) 116497. https://
doi.org/ 10.1016/J.INDCROP.2023.116497.
8. L. Bu, Y. Tang, Y. Gao, H. Jian, J. Jiang, Comparative characterization of milled wood lignin from furfural residues and
corncob, Chem. Eng. J. 175 (2011) 176184. https://doi.org/10.1016/J.CEJ.2011.09.091.
9. J. Seo, H. Kim, S. Jeon, S. Valizadeh, Y. Khani, B.H. Jeon, G.H. Rhee, W.H. Chen, S. Lam, M.A. Khan, Y.K. Park,
Thermocatalytic conversion of wood-plastic composite over HZSM-5 catalysts, Bioresour. Technol. 373 (2023) 128702.
https://doi.org/10.1016/J.BIORTECH.2023.128702.
INTERNATIONAL JOURNAL OF LATEST TECHNOLOGY IN ENGINEERING,
MANAGEMENT & APPLIED SCIENCE (IJLTEMAS)
ISSN 2278-2540 | DOI: 10.51583/IJLTEMAS | Volume XIII, Issue V, May 2024
www.ijltemas.in Page 44
10. X. Qi, Y. Shang, Z. Ding, W. Wei, Particularities and research progress of the cutting machinability of wood-plastic
composites, Mater. Today Commun. 37 (2023) 106924. https://doi.org/10.1016/J.MTCOMM.2023.106924.
11. L. Zhao, Y. Wei, F. Xi, Y. He, X. Wang, Experimental investigation on the flexural behavior of aluminum alloy-
reinforced wood plastic composite hollow members, Structures. 56 (2023) 104858. https:// doi.org/ 10.1016/J.ISTRUC.
2023.07.048.
12. C. Wang, C. Li, S. Zhu, D. Tu, L. Wu, Y. Chen, Y. Guo, Exploring an efficient non-destructive approach to characterize
damage behavior and crack propagation of highly-filled wood-plastic composites during three-point bending test, Constr.
Build. Mater. 364 (2023) 129920. https://doi.org/10.1016/J.CONBUILDMAT.2022.129920.
13. L.N. Hilary, S. Sultana, Z. Islam, M.K.U. Sarker, M.J. Abedin, M.M. Haque, Recycling of waste poly(vinyl chloride) fill
materials to produce new polymer composites with propylene glycol plasticizer and waste sawdust of Albizia lebbeck
wood, Curr. Res. Green Sustain. Chem. 4 (2021) 100221. https://doi.org/10.1016/J.CRGSC.2021.100221.
14. D. Zhang, X. Lin, Q. Zhang, X. Ren, W. Yu, H. Cai, Catalytic pyrolysis of wood-plastic composite waste over activated
carbon catalyst for aromatics production: Effect of preparation process of activated carbon, Energy. 212 (2020) 118983.
https://doi.org/10.1016/J.ENERGY.2020.118983.
15. L. Zhao, F.X. Doctor, Flexural performance of reinforced aluminumwoodplastic composite beam: An experimental
and numerical investigation, Thin-Walled Struct. 180 (2022) 109910. https://doi.org/10.1016/J.TWS.2022.109910.
16. D. Friedrich, Effects on heat storage from hot-pressing of wood-plastic composites for thermoformed climate-regulating
building skins, J. Energy Storage. 53 (2022) 105106. https://doi.org/10.1016/J.EST.2022.105106.
17. Z. Li, Y. Huang, Z. Zhu, H. Cheng, J. Zhao, M. Yu, W. Xu, Q. Yuan, T. He, S. Wang, Co-pyrolysis of sewage sludge
with polyvinyl chloride (PVC)/CaO: Effects on heavy metals behavior and ecological risk, Fuel. 333 (2023) 126281.
https:// doi. org/10.1016/J.FUEL.2022.126281.
18. M. Al-Rubaiai, X. Qi, Z. Frank, R. Tsuruta, U. Gandhi, K.J. Kim, X. Tan, Control-oriented Nonlinear Modeling of
Polyvinyl Chloride (PVC) Gel Actuators, IFAC-PapersOnLine. 54 (2021) 304309. https://doi.org/ 10.1016/ J.IFACOL.
2021.11.191.
19. X. Xu, D. Zhu, X. Wang, L. Deng, X. Fan, Z. Ding, A. Zhang, G. Xue, Y. Liu, W. Xuan, X. Li, J. Makinia,
Transformation of polyvinyl chloride (PVC) into a versatile and efficient adsorbent of Cu(II) cations and Cr(VI) anions
through hydrothermal treatment and sulfonation, J. Hazard. Mater. 423 (2022) 126973. https://doi.org/ 10.1016/ J.
JHAZMAT. 2021.126973.
20. J. Song, J. Wang, J. Sima, Y. Zhu, X. Du, P.T. Williams, Q. Huang, Dechlorination of waste polyvinyl chloride (PVC)
through non-thermal plasma, Chemosphere. 338 (2023) 139535. https://doi.org/10.1016/J.CHEMOSPHERE.2023.
139535.
21. M. Fashandi, S. Karamikamkar, S.N. Leung, H.E. Naguib, J. Hong, B. Liang, C.B. Park, Synthesis, structures and
properties of hydrophobic Alkyltrimethoxysilane-Polyvinyltrimethoxysilane hybrid aerogels with different alkyl chain
lengths, J. Colloid Interface Sci. 608 (2022) 720734. https://doi.org/10.1016/J.JCIS.2021.09.128.
22. O.A. Tafreshi, Z. Saadatnia, S. Ghaffari-Mosanenzadeh, T. Chen, S. Kiddell, C.B. Park, H.E. Naguib, Flexible and
shape-configurable PI composite aerogel films with tunable dielectric properties, Compos. Commun. 34 (2022) 101274.
https:// doi.org/10.1016/J.COCO.2022.101274.
23. M. Rabiei, A. Palevicius, R. Ebrahimi-Kahrizsangi, S. Nasiri, A. Vilkauskas, G. Janusas, New Approach for Preparing
In Vitro Bioactive Scaffold Consisted of Ag-Doped Hydroxyapatite + Polyvinyltrimethoxysilane, Polymers (Basel). 13
(2021) 1695. https://doi.org/10.3390/polym13111695.
24. M. Rabiei, M.S. Raziyan, R. Ebrahimi-Kahrizsangi, S. Nasiri, A. Palevicius, G. Janusas, A. Vilkauskas, Effects of 5
wt.% Polycaprolactone, Polyhydroxybutyrate and Polyvinyltrimethoxysilane on the Properties of Ag/Zn/Mg Alloy,
Mater. 2022, Vol. 15, Page 5421. 15 (2022) 5421. https://doi.org/10.3390/MA15155421.
25. S. Nasiri, M. Hosseinnezhad, M. Rabiei, A. Palevicius, G. Janusas, The effect of calcination temperature on the
photophysical and mechanical properties of copper iodide (5 mol%)doped hydroxyapatite, Opt. Mater. (Amst). 121
(2021) 111559. https://doi.org/10.1016/J.OPTMAT.2021.111559.
26. A. Bryś, J. Bryś, E. Ostrowska-Ligęza, A. Kaleta, K. rnicki, S. Głowacki, P. Koczoń, Wood biomass characterization
by DSC or FT-IR spectroscopy, J. Therm. Anal. Calorim. 126 (2016) 2735. https://doi.org/10.1007/S10973-016-5713-
2/ TABLES/1.
27. P.R. Kubade, R. Senanayake, Studies on thermo-mechanical properties of HNTs filled ABS/PVC composites, Mater.
Today Proc. 59 (2022) 248252. https://doi.org/10.1016/J.MATPR.2021.11.104.
28. F.L. Scholten, n. v. Veg-Gasinstituut, DSC investigations of PVC and PVC/CPE gas pipes, Thermochim. Acta. 93
(1985) 203206. https://doi.org/10.1016/0040-6031(85)85052-8.
29. C. Song, X. Zhang, Y. Ma, W. Yang, Synthesis internal-plasticized PVC copolymer resin from industrial application
view: Copolymerization of vinyl chloride with poly(ethylene glycol) monomethyl ether methacrylate via suspension
polymerization, Polymer (Guildf). 290 (2024) 126562. https://doi.org/10.1016/J.POLYMER.2023.126562.
30. H. Cao, W. Feng, H. Zeng, T. Jin, Y. Lin, L. Xie, X. Chai, K. Xu, G. Du, L. Zhang, A innovative application of lactose
cross-linked adhesive in plywood using hyperbranched network structure with high performance, React. Funct. Polym.
191 (2023) 105698. https://doi.org/10.1016/J.REACTFUNCTPOLYM.2023.105698.
31. T. Höfer, A. Rössler, O.I. Strube, Thermal debonding on demand for wood coatings via nitrocellulose-based primer,
Prog. Org. Coatings. 188 (2024) 108215. https://doi.org/10.1016/J.PORGCOAT.2024.108215.
INTERNATIONAL JOURNAL OF LATEST TECHNOLOGY IN ENGINEERING,
MANAGEMENT & APPLIED SCIENCE (IJLTEMAS)
ISSN 2278-2540 | DOI: 10.51583/IJLTEMAS | Volume XIII, Issue V, May 2024
www.ijltemas.in Page 45
32. I. Turku, A. Keskisaari, T. Kärki, A. Puurtinen, P. Marttila, Characterization of wood plastic composites manufactured
from recycled plastic blends, Compos. Struct. 161 (2017) 469476. https://doi.org/ 10.1016/J.COMPSTRUCT. 2016. 11.
073.
33. J. Gao, W. Lin, S. Lin, X. Zhang, W. Yang, R. Li, Environment-Friendly and Two-Component Method for Fabrication
of Highly Hydrophobic Wood Using Poly(methylhydrogen)siloxane, Polym. 2021, Vol. 13, Page 124. 13 (2020) 124.
https://doi.org/10.3390/POLYM13010124.
34. L.L. Wang, N. Li, T. Zhao, B. Li, Y. Ji, Magnetic Properties of FeNi3 Nanoparticle Modified Pinus radiata Wood
Nanocomposites, Polym. 2019, Vol. 11, Page 421. 11 (2019) 421. https://doi.org/10.3390/POLYM11030421.
35. R. Fu, C. Dong, Y. Zhang, C. Sun, R. Qu, C. Ji, Y. Zhang, PPTA-oligomer functionalized multiwalled carbon nanotubes
synthesized by “one-pot” method for reinforcement of polyvinyl chloride, J. Mater. Sci. 54 (2019) 11804–11817.
https://doi.org/10.1007/S10853-019-03730-2/METRICS.
36. T. Deng, S. Li, P. Jia, N. Yao, H. Ding, L. Xu, Y. Zhang, X. Yang, M. Li, Self-Plasticized PVC Prepared by Introducing
Fatty Acid to the PVC with Triglycidyl Isocyanurate as an Intermediate Bridge, ACS Omega. 7 (2022) 3569435704.
https://doi.org/10.1021/ACSOMEGA.2C03655/SUPPL_FILE/AO2C03655_SI_001.PDF.
37. G. Nguila Inari, M. Pétrissans, S. Dumarcay, J. Lambert, J.J. Ehrhardt, M.S. ˇernek, P. Gérardin, Limitation of XPS for
analysis of wood species containing high amounts of lipophilic extractives, (n.d.). https://doi.org/10.1007/s00226-010-
0324-8.
38. J. Bañuls-Ciscar, D. Pratelli, M.L. Abel, J.F. Watts, Surface characterisation of pine wood by XPS, Surf. Interface Anal.
48 (2016) 589592. https://doi.org/10.1002/SIA.5960.
39. R. de Abreu Neto, J.T. Lima, L.M. Takarada, P.F. Trugilho, Effect of thermal treatment on fiber morphology in wood
pyrolysis, Wood Sci. Technol. 55 (2021) 95108. https://doi.org/10.1007/S00226-020-01238-6/METRICS.
40. M.E. mez Yepes, L. V. Cremades, Characterization of Wood Dust from Furniture by Scanning Electron Microscopy
and Energy-dispersive X-ray Analysis, Ind. Health. 49 (2011) 492500. https://doi.org/10.2486/INDHEALTH.MS1204.
41. Chapter 1 Hooke’s law, Poisson’s relation and waves along thin bars, Methods Geochemistry Geophys. 39 (2005) 182.
https://doi.org/10.1016/S0076-6895(05)80003-4.
42. S. Kopylov, Z.B. Chen, M.A.A. Abdelkareem, Acceleration based ground-hook control of an electromagnetic
regenerative tuned mass damper for automotive application, Alexandria Eng. J. 59 (2020) 49334946. https://doi.org/
10. 1016/ J.AEJ. 2020.09.010.